Iranian Classification Society Rules

< Previous | Contents | Next >

Section 12 Synthetic Fibre Ropes


1201. Application


1. The requirements in this Section apply to the tests and inspection for the approval of manufacturing process of synthetic fibre ropes specified in Pt 4, Ch 8, 603. of the Rules.


2. Where it is difficult to comply with test methods and evaluation criteria specified in this Section, the decision may apply to standards authorized by the Society. (officially recognized establishment)


1202. Data to be submitted

The Society may request to submit the data about following tests for raw textiles for synthetic fi- bre ropes:

(1) Linear strength and elongation tests

(2) Chemical resistance test


1203. Approval tests


1. Selection of test samples

Test pieces are to be taken suitable length from end of each length of synthetic fibre ropes. The number of rope to be taken for tests is to be as specified in Table 2.12.1.

2. Approval tests and acceptance criteria

(1) The approval test is to be carried out on each kind of ropes under application for each manu- facturing factory. The details of approval test are to be as indicated in Table 2.12.1 and the test is to be carried out in the presence of the Surveyor. Provided, however, approval test is carried

out in the presence of inspector of the organization authorized by the Society (officially nized establishment), the test witnessed by the Surveyor of the Society may be omitted.

recog-


Kind of rope Diameter

of test rope

Vinylon rope polyester rope nylon rope


Polyethylene rope polypropylene rope


12 ~ 24 mm

Wet condition(1)

Wet condition(3)

Dry condition(2)

Dry condition(2)


40 ~ 60 mm

Wet condition(1)

Wet condition(3)

Dry condition(2)

Dry condition(2)

NOTES:

(1) The test specimen is to be soaked in water at normal temper- ature for a period of 30 m inutes or more, then taken out and subjected to tensile test at room temperature.

(2) The test specimen in dry condition is to be subjected to tensile test at room temperature.

(3) The test specimen is to be soaked in warm water at temper- ature of 35 ± 2°C for a period of 30 m inutes or more, then

taken out and immediately subjected to tensile test at room temperature.

Table 2.12.1 Approval Test Items and Acceptance Criteria for synthetic fibre ropes


Test item

Test method

Acceptance criteria

Construction

& Diameter

Construction and diameter of synthetic fibre ropes are to be measured in accordance with Pt 4, Ch 8, Sec 6 of the Rule.

To comply with the Pt 4, Ch 8, Sec 6 of the Rule.


Tensile tests in

wet and dry conditions

(1) Tensile tests on three each test specimens are to, in prin- ciple, be carried out for each of the test conditions given in Table below and breaking strength and elongation are to be measured. For rope having diameter higher than 60mm, one additional tensile test specimen is to be taken from the rope of maximum diameter.

(2) The gauge length of the test specimen is to be 30 times or more of the rope diameter, however it needs not to ex- ceed 1 meter.

image


(1) Except on cases with vinylon and nylon in wet condition, respective breaking loads are to satisfy the requirements specified in Pt 4, Ch 8, Sec 6, of the Rules.

(2) The breaking loads of vinylon and nylon in wet conditions are to be 80 % or more and 90 % or more respectively of the values specified in above (1)

(3) Values with respect to elongation are to be for reference only.


Guidance for Approval of Manufacturing Process and Type Approval, Etc. 2015 51

image

Ch 2 Approval of Manufacturing Process Ch 2, Sec 12

image



Kind of rope

Residual abrasion strength ratio (%)

Vinylon rope

min. 50

Polyethylene rope

min. 55

Polyester rope

min. 55

Polypropylene rope


min. 55

Nylon rope

min. 55

Table 2.12.1 Approval Test Items and Acceptance Criteria for synthetic fibre ropes (continued)


Test item

Test method

Acceptance criteria


Abrasion resistance tensile test

(1) A total of six test specimens are to be taken from ropes with diameter from 12 to 24 mm. Three of them are to be set in the abrasion resistance testing machine with the following particulars, and are to be subjected to repeated strokes for 500 times.

Stroke: 200~300 mm

Abrasion speed: 50 strokes/min.

Abrasion surface: Grinder with particle size No. 120

Tensile load : 98 N

(2) Those three tested specimens together with other three non-tested specimens are to be placed in a thermostatic oven kept at a

temperature of 20 °C and a humidity of 65 %, and left there for one hour.

(3) They are then to be taken out, and be subjected to tensile tests for measuring the tensile strength and elongation, whereby the

strength values of the rope before and after abrasion are to be compared.

(4) For other test conditions than those shown above, they are to be considered appropriate by the Society.


The ratio of the residual abrasion strength to the strength without abra- sion (the residual abrasion strength ra- tio) is to satisfy the values given in table below.


Weather resistance test

(1) A total of six test specimens are to be taken from ropes with diameter from 12 to 24 mm. Three of these test specimens are to be placed in the weather resistance test machine controlled to the following conditions where they are to be left for 200 hours or more.

Weathering light : Sunshine carbon arc light or ultraviolet carbon arc light (KS F 2274 (Recommended Practice for Accelerated Artificial Exposure of Plastics Building

Materials))

Temperature of black panel : 63 ± 1 °C

Period of water spray : 18 min/2 hours

(2) The six test specimens including those three non tested speci- mens are then to be placed in a thermostatic oven kept at a

temperature of 20 °C and a humidity of 65 %, and left there for one hour. These test specimens are to be taken out, tensile strength and elongation are to be measured, and the strength af- ter the weathering resistance test and that of the test specimens not subjected to such weathering resistance test are to be compared.


The ratio of the former to the latter (the residual weathering strength ratio) is to satisfy the values given in table below.



Kind of rope

Residual weathering strength ratio (%)

Vinylon rope

min. 90

Polyethylene rope

min. 80

Polyester rope

min. 90

Polypropylene rope


min. 80

Nylon rope

min. 80

(2) The procedures of the test for raw textiles for synthetic fibre ropes refer to the Table 2.12.2


Table 2.12.2 Approval Test Items and Acceptance Criteria for raw textiles for synthetic fibre ropes


Test item

Test method

Acceptance criteria


Linear strength and elongation tests

(1) The test procedures of filament and split are to be in accordance with KS K 0412, and those of span are to be correspondingly on accordance with KS K 0475 (Testing Method for Tensile Strength of Spun Yarns).

(2) The number of test specimens used in the test is to be 10 and average value of the linear strength and elongation on these test specimens are to be

obtained.


The average value of lin- ear strength and elonga- tion obtained are to com- ply with the requirements given in Table 2.12.3.


Chemical re- sistance test

(1) The chemical resistance tests are to comprise alkali-resistance test and acid-re- sistance test.

(2) In alkali-resistance test, the test specimen is to be socked in 10% caustic so- da solution at a temperature 20±2°C for a period of 24 hours, whereas in

acid-resistance test, the test specimen is to be socked in 10% acid solution at

a temperature 20±2°C for a period of 24 hours, and then rinsed with water,

and the linear strength is to be measured by the same method as in (1)

above.

(3) The number of test specimens are to be 10 for each chemical solution. The linear strength is to be converted into the value of residual strength ratio of chemical resistance by following equation.


linear strength(g) after chemical processing

Residual chemical resistance strength ratio = --------------------------------------------------------- × 100(%)

linear strength(g) before chemical processing


These average values are to satisfy the values giv- en in Table 2.12.3.


52 Guidance for Approval of Manufacturing Process and Type Approval, Etc. 2015

image

Ch 2 Approval of Manufacturing Process Ch 2, Sec 12

image


Table 2.12.3 Standard Tensile Strength Values for Raw Textiles



Kind of raw textiles


Mechanical properties

Residual chemical resistance strength ratio(%)

Linear strength(g/D)

Linear elongation (%)

10% sulphuric acid

10% caustic soda


Vinylon


for Grade 1

Span, mono- filament


4.0 min.


9 ~ 18


90 min.


90 min.

for Grade 2

Multi-filament

6.0 min.

9 ~ 18

90 min.

90 min.


Polyethyl ene

for Grade 1

Mono-filament

6.5 min.

5 ~ 25

90 min.

90 min.

for Grade 2

Mono-filament

8.5 min.

5 ~ 15

95 min.

95 min.

Polyester

Multi-filament

5.5 min.

10 ~ 20

90 min.

90 min.


Polyprop ylene


for Grade 1

Span

4.5 min.

10 ~ 20

90 min.

90 min.

Mono-filament

6.0 min.

10 ~ 20

90 min.

90 min.


for Grade 2

Multi-filament

6.5 min.

15 ~ 25

90 min.

90 min.

Special mono- filament


6.0 min.


5 ~ 15


90 min.


90 min.

Special multi-filament


5.5 min.


5 ~ 15


90 min.


90 min.

Split

4.0 min.

5 ~ 15

90 min.

90 min.

Nylon

Multi-filament

6.5 min.

15 ~ 30

80 min.

80 min.

NOTE:

g/D signifies gram/denier


1204. Yarn test

In case where manufacturer's testing equipment does not have enough capacity for tensile test of fi- bre rope, yarn test may be substitute for tensile test specified in Table 2.12.1 provided that yarn test specimens are to be taken from fibre rope strand in question and, for calculating the breaking load, realization factor authorized by the Society shall be multiplied to the average yarn test value.


Guidance for Approval of Manufacturing Process and Type Approval, Etc. 2015 53

image

Ch 2 Approval of Manufacturing Process Ch 2, Sec 13

image